| 斷裂伸長率 | 850% | 拉伸強(qiáng)度 | 68MPa | 密度 | 0.919g/cm3 |
| 熔體流動速率 | 0.9g/10min | 維卡軟化點 | 102℃ | 用途級別 | 薄膜級,光學(xué)級 |
| 規(guī)格級別 | 薄膜 |
|
|
產(chǎn)品簡述
| 斷裂伸長率 | 850% | 拉伸強(qiáng)度 | 68MPa | 密度 | 0.919g/cm3 |
| 熔體流動速率 | 0.9g/10min | 維卡軟化點 | 102℃ | 用途級別 | 薄膜級,光學(xué)級 |
| 規(guī)格級別 | 薄膜 |
詳細(xì)數(shù)據(jù)
訂購指南
| 性能項目 | 試驗條件[狀態(tài)] | 測試方法 | 測試數(shù)據(jù) | 數(shù)據(jù)單位 | ||
| 基本性能 | 密度 | ASTM D-1505 | 0.919 | g/cm3 | ||
| 熔體流動速率 | ASTM D-1238 | 0.9 | g/10min | |||
| 物理性能 | 薄膜厚度 | 25 | µm | |||
| 機(jī)械性能 | 尖頭沖擊強(qiáng)度 | ASTM D-1709 | 5 | g/μm | ||
| 拉伸斷裂強(qiáng)度 | MD | ASTM D-882 | 400 | Kg/cm2 | ||
| TD | ASTM D-882 | 700 | Kg/cm2 | |||
| 撕裂強(qiáng)度 | MD | ASTM D-1004 | 130 | Kg/cm | ||
| TD | ASTM D-1004 | 120 | Kg/cm | |||
| 斷裂伸長率 | MD | ASTM D-882 | 700 | % | ||
| TD | ASTM D-882 | 850 | % | |||
| 撕裂彈性率 | MD | ASTM D-882 | 2200 | Kg/cm2 | ||
| TD | ASTM D-882 | 3100 | Kg/cm2 | |||
| 拉伸屈服強(qiáng)度 | MD | ASTM D-882 | 140 | Kg/cm2 | ||
| TD | ASTM D-882 | 130 | Kg/cm2 | |||
| 熱性能 | 維卡軟化點 | ASTM D-1525 | 102 | ℃ | ||
| 低溫脆化溫度 | ASTM D-746 | <-80 | ℃ | |||