| 斷裂伸長率 | 781% | 拉伸強度 | 10MPa | 密度 | 0.925g/cm3 |
| 熔體流動速率 | 0.7g/10min | 維卡軟化點 | 95℃ | 用途級別 | 薄膜級 |
| 規(guī)格級別 | 薄膜 | 加工級別 | 擠出級 |
|
|
產(chǎn)品簡述
| 斷裂伸長率 | 781% | 拉伸強度 | 10MPa | 密度 | 0.925g/cm3 |
| 熔體流動速率 | 0.7g/10min | 維卡軟化點 | 95℃ | 用途級別 | 薄膜級 |
| 規(guī)格級別 | 薄膜 | 加工級別 | 擠出級 |
詳細(xì)數(shù)據(jù)
訂購指南
| 性能項目 | 試驗條件[狀態(tài)] | 測試方法 | 測試數(shù)據(jù) | 數(shù)據(jù)單位 | |||||
| 基本性能 | 熔體流動速率 | 190℃/2.16kg | ASTM D-1238 | 0.70 | g/10min | ||||
| 密度 | ASTM D-1505/2839 | 0.925 | g/cm3 | ||||||
| 機械性能 | 拉伸斷裂強度 | ASTM D-882 |
|
MPa | |||||
| 斷裂伸長率 | ASTM D-882 |
|
% | ||||||
| 1%正割模量 | ASTM D-882 |
|
MPa | ||||||
| 埃爾曼多夫撕裂強度 | ASTM D-1922 |
|
gf | ||||||
| 落鏢沖擊強度 | ASTM D-1709 | 96 | gf/50%f | ||||||
| 摩擦系數(shù) | 動態(tài) | ASTM D-1894 | 0.08 | ||||||
| 拉伸斷裂強度 | ASTM D-638 | 10 | MPa | ||||||
| 斷裂伸長率 | ASTM D-638 | 781 | % | ||||||
| 熱性能 | 熔點 | ASTM D-3417/3418 | 114 | ℃ | |||||
| 維卡軟化點 | 10N/120℃/h | ASTM D-1525 | 95 | ℃ | |||||
| 光學(xué)性能 | 霧度 | ASTM D-1003 | 6 | % | |||||
| 光澤度 | 60° | ASTM D-2457 | 10.1 | % | |||||