| 斷裂伸長率 | 790% | 拉伸強度 | 29MPa | 密度 | 0.947g/cm3 |
| 熔體流動速率 | 0.35g/10min | 用途級別 | 薄膜級 | 規(guī)格級別 | 薄膜 |
| 缺口沖擊強度 | 165 | 加工級別 | 擠出級 |
|
|
產(chǎn)品簡述
| 斷裂伸長率 | 790% | 拉伸強度 | 29MPa | 密度 | 0.947g/cm3 |
| 熔體流動速率 | 0.35g/10min | 用途級別 | 薄膜級 | 規(guī)格級別 | 薄膜 |
| 缺口沖擊強度 | 165 | 加工級別 | 擠出級 |
詳細數(shù)據(jù)
訂購指南
| 性能項目 | 試驗條件[狀態(tài)] | 測試方法 | 測試數(shù)據(jù) | 數(shù)據(jù)單位 | ||
| 基本性能 | 熔體流動速率 | 190℃/5.0kg | ASTM D-1238 | 0.35 | g/10min | |
| 熔體流動速率 | 190℃/21.6kg | ASTM D-1238 | 8.5 | g/10min | ||
| 密度 | ASTM D-1505 | 0.947 | g/cm3 | |||
| 機械性能 | 最終強度 | MD | ASTM D-882 | 84 | MPa | |
| TD | ASTM D-882 | 49 | MPa | |||
| 屈服拉伸強度 | MD | ASTM D-882 | 43 | MPa | ||
| TD | ASTM D-882 | 29 | MPa | |||
| 斷裂伸長率 | MD | ASTM D-882 | 580 | % | ||
| TD | ASTM D-882 | 790 | % | |||
| 缺口沖擊強度 | ASTM D-1709 | 165 | gf/50%F | |||
| 埃爾曼多夫撕裂強度 | MD | ASTM D-1922 | 5 | kgf/cm | ||
| TD | ASTM D-1922 | 57 | kgf/cm | |||
| 穿刺強度 | Braskem Method | 78 | J/M | |||
| 其它性能 | 最小推薦厚度 | 13 | μm | |||